To achieve this color - lay in PP - Coal, cure to specified time / temp.
You MUST add large red metal flake .25 ounce to 1lb of clear, add a pinch of silver flake for more colors in the metallic if you wish, we did use a tiny amount of silver flake in this shoot.
Warm the parts to 150F - and shoot the clear and metal flake while warm. Cure out at 390F metal temp for 10-13 minutes.
It will produce a slightly textured satin finish with an almost chameleon result, hints of maroon, plum, smoke etc. depending on the lighting conditions.